<p>In this case the first method (Exercise No. 1) is to be used whenever possible, as it gives a much smoother joint than the second method. The directions given will describe the adaptation of this method to the problem: if the second method must be used on account of awkward shape, etc., of the work, the modifications required will be obvious to any one who has learned to make the joint by the first method.</p>
<p>After sealing or corking one end of the larger tube, the other end is drawn out to form a tail as described on page 9, taking care to have the tube uniformly heated, and to draw the tail rapidly enough so that the cone is short, as indicated in <em>a</em>, Fig. 8. The tube is now rotated, a small flame directed against the cone at right angles to an element of it, and it is allowed to shrink a little, as indicated in <em>b</em>, Fig. 8, so that its walls will thicken. When the tail is cut off, at the dotted line, the diameter of the opening and the thickness of the walls at that point should correspond with the dimensions of the tube to be sealed on. As the glass is hot, the scratch for cutting it must be made with a file (moisten the edge!), and it often will not break square across. Before proceeding to seal on the small tube, any large projections on the cut end are best removed, by warming the cut surface a little, directing the small flame upon each projection in turn and touching it with a warm scrap of glass. It will adhere to this and may then be removed by rotating this scrap a little so as to wind up the projection on it, and then drawing it off, while the flame is still playing on the spot. This must be done rapidly and care taken not to soften the main part of the cone.<br>
<br>
</p>
<div> <img src="images/i034.png" alt="" title="" width="400" height="256"> Fig. 8.—Joining two tubes of different diameters. <br>
<br>
</div>
<p>The large tube is now taken in the left hand, the small one in the right, the ends heated and joined in the usual manner, taking care not to get any larger lump at the joint than necessary. A small flame is now directed on the cone at right angles to its elements as before, and the tube rotated so as to heat the whole circumference. The flame should be just large enough to heat the whole of the cone. As the latter shrinks, the lump at the joint is brought into the edge of the flame, and it and a very little of the small tube allowed to shrink with the cone.</p>
<p>When well shrunk and heated to blowing temperature the joint is removed from the flame and blown gently with careful rotation, pushing the tubes together a little when the blowing is about finished, so that the cone becomes a short thick half-bulb, as shown in <em>d</em>, Fig. 8. This corresponds to the first thick bulb in the first method (<em>d</em>, Fig. 6), and is treated similarly. It is again heated and shrunk, taking care not to involve either the large tube or the small one in the shrinking, blown quickly to about the same shape as before, (<em>d</em>, Fig. 8), and then gently drawn out into a smooth cone (<em>e</em>), exactly as in the first exercise. Care should be taken not to draw too rapidly or too far, as then the resulting cone (<em>f</em>) is weaker than it should be, and does not look well.</p>
<p><strong>Discussion.</strong>—The beginner will find that this operation is best learned on two tubes which are not too nearly of the same diameter. A tube about 5⁄8 inch in diameter and one a little less than 1⁄4 inch will be suitable. Both should have moderately heavy walls (1⁄16 inch or a trifle over for the large tube, and a trifle less for the small one) but the large tube should not be too heavy or else it will be hard to prevent melting down too much of the small tube, and getting this drawn out too thin during the process. One of the troublesome features of this exercise is the difficulty of rotating two tubes of different diameters with the same angular velocity, so as not to twist the joint. Another difficulty is found in getting the cone uniformly heated to blowing temperature without overheating and overshrinking the small tube. The reason for this is obviously the much greater circumference of the cone, especially at its large end, so that relatively much less of it is being heated at any time. The beginner is also inclined to start with too long a cone, or else heat so much of the large tube that part of its glass is included in the cone, with the result that in order to get the right wall-thickness the cone must be made too long (<em>g</em>, Fig. 8). This does not look well, and usually will be irregular in shape.</p>
This piece is part of Laboratory Manual Of Glass-blowi. Explore the full collection for more from this work.