This exercise is most easily learned on tubing with an exterior diameter
of 1/4 inch, or a little less, having moderately heavy walls. A piece of
such tubing is heated before the blow-pipe at a point ten or twelve
inches from the end, and there drawn out to a capillary as previously
described (page 9). The capillary is sealed off about two inches from
the main tube, and the latter is cut near the middle. Care should be
taken to get square ends where the cut is made (page 7). The flame is
now so regulated that it is a little broader than the diameter of the
tube, the sealed half of the tube taken in the left hand and the other
half in the right. The open end of the sealed part and one of the ends
of the other part are now held in opposite sides of the flame, inclined
at a slight angle to one another as indicated in Fig. 5, and rotated and
heated until the surfaces of both ends are just softened. The two ends
are then carefully and quickly brought together (a, Fig. 6), removed
from the flame and pulled apart a little, to reduce the lump formed at
the joint as much as possible, as indicated in b. The joint is then
tested by blowing into the open end of the tube to see if it is tight.
If so, the flame is reduced to half or less than half of its former
size, and the joint heated in it, holding the tube and continually
rotating it as directed in the last chapter (page 13).
As the tube softens and tends to shrink, the two ends are pressed
together a little and the walls allowed to thicken slightly, as in c.
It is then quickly removed from the flame and gently blown as indicated
in d, continuing the rotation of the tube during the blowing, and at
the same time pressing the ends of the tube together a little so as to
make a short thick-walled bulb. The joint is then returned to the
flame and reheated, rotating as before, shrinking to about the shape of
e. When this stage is reached, the glass should be very hot and fluid,
and the mass of hot glass thick enough to remain at its working
temperature for about five seconds after removal from the flame. The
glass is now reblown as indicated in f, to form a bulb having walls of
practically the same thickness as the original tube. As soon as the bulb
is blown, the tube is removed from the mouth, held horizontally in front
of the worker, and gently drawn out to form one continuous tube, as
indicated in g. During both the blowing and drawing of this bulb the
rotation must be continued, and both blowing and drawing must be
carefully regulated so that the resulting tube may have the same
internal and external diameter at the joint as elsewhere.
=Discussion.=--In making the original joint, (a, Fig. 6), care should
be taken that the lump formed is as small as possible so that it may be
entirely removed during the subsequent operations. For this reason, only
the very tip ends of the two pieces of tubing are held in the flame, and
the softening should not extend more than 1/16 inch down the tube. As
soon as the ends are sufficiently soft to stick together, they are made
to do so. The first drawing of the tube (b) should take place
immediately, and reduce the lump as much as possible without making the
adjacent walls of the tube thin. The whole purpose of the rest of the
manipulation is to absorb or "iron out" the lump at the joint. For this
reason, care is taken that this lump is always in the center of the
flame while the joint is being heated, and a small flame is used so
that little of the main tube may be softened. During the first shrinking
of the joint (c) the walls next the lump, being thinner than it is,
reach the softening temperature first and are thickened by the slight
pushing together of the ends, so that they taper from the lump to the
unchanged wall. Upon blowing this joint, these thickened walls blow out
with the lump, but as they are thinnest next the unchanged tube, they
stiffen there first. Then as the thicker parts are still hot, these blow
out more, and with the lump make a more or less uniform wall. By this
first operation most of the lump will have been removed, provided it was
not too large at first, and the tube was hot enough when it was blown.
Beginners almost invariably have the glass too cool here, and find
difficulty in blowing out a satisfactory bulb. Under such circumstances
the lump will be scarcely affected by the operation.
During the shrinking of this bulb, the thinner parts of course are the
first to reach the softening point, and thus contract more than the
thick parts, so that practically all of the lump can be absorbed, and a
uniformly thickened part of the tube left as in e. When this is just
accomplished, the second bulb must be blown during one or two seconds,
and the tube then drawn out as described, so as to change the bulb to a
tube. The drawing must proceed with care: portions nearest the unchanged
tubes are the first to reach the proper diameter, and must be given time
to just set at that point before the center of the bulb is finally drawn
into shape. The drawing is perhaps best done intermittently in a series
of quick pulls, each drawing the tube perhaps 1/16 inch, and each taking
place as the thumbs and first fingers grasp the tube for a new turn in
the rotation. If the tube is not rotated during the blowing, the bulbs
will be lop-sided and it will be impossible to get a joint of uniform
wall-thickness; if rotation is omitted during the drawing, the tube
will almost invariably be quite crooked.
If the lump still shows distinctly after the operations described, the
cross-section of the tube will be as in h, and the tube will be likely
to break if ever reheated at this point after it becomes cold. The
operations d, e, f, and g may be repeated upon it, and it may be
possible to get it to come out all right.
Care must be taken not to blow the bulbs d and f too thin as they
then become very difficult to handle, and the joint is usually spoiled.
The wall-thickness of these bulbs must never be much less than that of
the original tube. If the joint as completed has thinner walls than the
rest of the tube, it will be more easily broken. It should be remembered
that the length of the finished tube must be exactly the same as that of
the original piece, if the walls of the joint are to be of their
original thickness. Therefore the pushing together during the two
operations c and d must shorten the tube just as much as the final
drawing (f to g) lengthens it.
The interval between the removal of the work from the flame and the
beginning of the blowing must be made as short as possible, or else the
portions next the main parts of the tube will set before they can be
blown out, and cause irregular shrunken areas.
This piece is part of Laboratory Manual Of Glass-blowi. Explore the full collection for more from this work.