The method described in Exercise No. 1 is very satisfactory for joining
short lengths of straight tubing, but becomes inconvenient or impossible
when the pieces are long or bent, on account of the difficulty in
uniformly rotating such work. In such cases, this second method is
used. It does not usually give as smooth and pretty a joint as the first
method, and takes a little longer.
The joint is begun exactly as in the first method, and the manipulation
is the same until after the preliminary tight joint (b, Fig. 6) is
made. The flame is reduced as usual, but instead of rotating the tube in
the flame, only one part of the circumference is heated, and this is
allowed to shrink thoroughly before blowing. It is then blown gently so
that it becomes a slight swelling on the tube, and the operation
repeated on an adjoining part of the joint. Three or four repetitions of
the operation will usually cover the whole circumference of the joint,
in a small tube, the result being a swelling roughly similar to the
first thick bulb in the first method (d, Fig. 6). If all the lumps of
the original joint have not been removed by this operation, it may now
be repeated upon such parts as may require it. The thickness of the wall
in the bulb should be about the same as that in the original tube. The
whole of the expanded joint is now heated as uniformly as may be until
soft enough so that it begins to shrink a little, and the swelling is
gently drawn down to the same diameter as the main tube, as in the first
case. Any irregularities in the finished joint may be corrected by local
reheating, shrinking or blowing as required.
=Discussion.=--In using this method, especially with larger sizes of
tubing, it is very important to keep the whole circumference of the
joint hot enough during the operation so that it does not crack apart at
the part which has not yet been worked. For that reason the first
heating, shrinking and blowing should be performed as quickly as
possible, leaving the resulting irregularities to be corrected later,
rather than attempting to reblow the same part of the joint several
times in succession until it is satisfactory. Care must be taken in this
as in the first method that the blowing follows immediately upon the
completion of the shrinking and removal of the object from the flame:
delay in blowing will cause shrunken places where the joint meets the
original tubes, on account of the cooling and setting of the glass
before it was blown. Most beginners err in being afraid to shrink the
part of the joint enough before blowing it. On small tubing, the
shrinkage may often extend so far that the inner surface of the shrunken
part reaches the center of the tube. Insufficient shrinking results in
failure to remove the lump formed at the original joint. It is often of
advantage, after blowing out part of the joint, to allow that part a few
seconds to set before going on with the rest, keeping the whole joint
warm meanwhile in or near the smoky flame. This helps to prevent the
twisting of the joint, or other distortion incident to the handling of a
piece of work of awkward shape.
In making a joint on a very long or heavy piece by this method, it is
often advantageous to attach a piece of rubber tubing to the open end,
hold the other end of this tubing in the mouth during the process, and
blow through it, rather than attempt to bring the end of the glass up to
the mouth. This enables one to keep closer watch on the joint, and avoid
drawing it out or distorting it in handling. On the other hand, the
rubber tube is an inconvenience on account of its weight and the
consequent pull on the end of the apparatus, and makes rotation
difficult.
This piece is part of Laboratory Manual Of Glass-blowi. Explore the full collection for more from this work.