<p>The operations involved are two: the blowing of a short side tube on a piece of tubing, and sealing another piece of tubing on this, by what is essentially the second method as just described.<br>
<br>
</p>
<div> <img src="images/i031.png" alt="" title="" width="230" height="400"> Fig. 7.—The "tee" tube. <br>
<br>
</div>
<p>The two pieces of tubing to be used each have one end cut square and the other sealed in the usual manner. The longer of the two is now heated at the point at which the joint is to be made, until it begins to color the flame. A small flame is used, and the tube rotated until the flame begins to be colored, when the rotation is stopped, and only one spot heated until a spot the diameter of the tube to be sealed on has become red hot and begun to shrink. This is now gently blown out into a small bulb, as in <em>a</em>, Fig. 7, and it will be noted that this bulb will have walls tapering from the thick walls of the tube to a very thin wall at the top. The sides of this bulb, below the dotted line, are to form the small side tube to which the main side tube is to be sealed. The top of the bulb is now softened by directing a small flame directly upon it, and as soon as it shrinks to the level indicated by the dotted line, it is removed from the flame and quickly blown out to form a thin bulb, as indicated in <em>b</em>, Fig. 7. This will usually be so very thin that a stroke of the file or glass-knife will break it off at the dotted line, leaving the side tube, to which the short piece of tubing is now sealed according to the second method (Exercise No 2). In doing this, care is taken to direct the flame partly on the main tube in the two crotches, so that both tubes blow out a little and give space for the gases to turn in, as indicated in <em>c</em>, Fig. 7, and at the same time increase the mechanical strength of the job. On the other hand, care is taken not to deform the main tube, and not to produce such a bulge or bulb at the joint as will prevent the finished tube from lying flat on a table.</p>
<p><strong>Discussion.</strong>—Most beginners tend to err in the first steps of this operation, by blowing too hard and too long when blowing out the little bulb. The result is a large, very thin bulb, which breaks off in such a way as to leave a hole in the main tube, occupying nearly half the circumference of the tube at that point, instead of the neat side tube which they should have. It is not difficult to seal a tube on this side tube, but it is very difficult to seal a tube into a hole in another tube. Care should be taken here, as in the two previous exercises, that the lump obtained at the joint when the two tubes are put together is made as small as possible, and reduced if possible by gently drawing on the side tube as soon as the tubes have actually joined. It is much easier to prevent the formation of a lump at the joint than it is to remove the lump after it is formed. The remarks previously made about blowing quickly after removing the work from the flame apply here with especial force. A "tee" tube, from its very nature, is exposed to a good many strains, so care must be taken that the walls of the joint are of uniform thickness with the rest of the tube.</p>
<p>The beginner will find it easiest to make this tube out of two pieces of the same tube, about 1⁄4 inch in diameter. Larger or smaller tubing is usually more difficult. If tubing much more than 1⁄4 inch is used, the whole joint, including part of the main tube, must be heated nearly to the softening point at the close of the operation, and well annealed, as described in Chapter 1 (page 3) or it will be almost certain to crack. In the larger sizes of tube it will be necessary to heat the whole circumference of the main tube frequently during the operation, to prevent it from cracking.</p>
<p>In sealing a small tube on the side of a large one, it is usually advisable, after warming the spot where the joint is to be made, to attach a small drop of glass to the tube at that point, and direct the flame upon that, thus supplying at the same time both a definite point to be heated and an extra supply of glass for the little side tube which is desired. In this way it is also easier to blow out a side tube with a sufficiently small diameter. If the diameter of this tube should be much greater than that of the small tube, the latter may be enlarged with a carbon or a flanging tool.</p>
This piece is part of Laboratory Manual Of Glass-blowi. Explore the full collection for more from this work.