Closed Tubes For Heating Under Pressure

(Carius method for determination of the halogens and sulphur.) In this

(Carius method for determination of the halogens and sulphur.) In this

case the tubing used must have thick walls (usually about 3/32 inch) to

withstand the pressure. Its external diameter is usually about 3/4 inch.

One length will usually make two tubes of standard length for the cannon

furnace. Especial care must be taken in heating and cooling it on

account of the thick walls. A length is gradually warmed in the center,

finally heated at that point until soft, drawn out, cut apart and

annealed. Taking one of the pieces, the cone is carefully heated and

shrunk, as in Exercise 4, until its walls are as thick as those of the

main tube. A flame with a little tinge of yellow should be used for this

operation to prevent devitrification (page 2), as the thick glass

shrinks slowly. The tail is now drawn off and the whole end heated and

gently blown several times to make a rounded end, like a test-tube, with

walls as thick as those of the main tube. This must be carefully

annealed. It is more important that the walls be thick than that the end

be nicely rounded: it may indeed be left somewhat conical in shape.

At a point about two inches from the open end of the tube, it is slowly

warmed and finally heated to the softening point. Grasping the open end

with a pair of crucible tongs, it is cautiously pulled out, a little at

a time, usually during rotation in the flame, to make a constriction of

moderate wall-thickness, but of sufficient internal diameter to admit

the tube containing the substance. After annealing this, cooling and

cleaning the tube, the acid and salt are introduced (the former by means

of a long-stemmed funnel) and the tube is inclined and rotated about its

axis so that the acid wets its surface about half way up from the

bottom. The substance is now weighed out in a piece of thin-walled glass

tubing, closed at one end, and about two inches long. Inclining the

large tube at a suitable angle, the small one is introduced, closed end

first, and allowed to slide down the walls of the large tube until it

reaches the place where the acid has wet the tube. Here it will stop,

and if the tube is kept inclined during the rest of the operation it

will roll around inside the tube at this point and thus not get down

where any acid is likely to get into it and produce any pressure by

decomposing it before the open end of the tube is sealed. Now the tube

is held in an inclined position, taking care that the acid does not

reach up to the substance, the constricted portion cautiously warmed and

shrunk. It is finally shrunk and drawn out into a somewhat elongated

cone, with walls as thick as the rest of the tube, and when this is

accomplished the end of the cone is sealed and the waste piece drawn

off. Anneal with great care, and cool in such a position that the acid

cannot reach the hot glass. The shrinking of this cone takes a good deal

of patience, and is one of the most important parts of the process. If

the walls are left too thin, the tube may burst when heated, and the

whole labor is lost. If care is taken, the same tube can be used for a

number of determinations, until it becomes quite short.