Glass Rod

Joints, tees, etc., in glass rod are made on the same principle as in

Joints, tees, etc., in glass rod are made on the same principle as in

tubing, except that of course they cannot be blown, and regularity must

be obtained by accumulating a small mass of uniformly heated glass, and

then drawing it to a suitable rod, on the same principle as Exercise No.

1.

Great care must be taken in heating and cooling this, as in the case of

the capillary tubing, and for the same reasons.

By joining pieces side by side, pressing with carbon plates or a plate

and a rod, and other suitable manipulations, stirrers, spatulas, and

other objects may easily be made from rod, and its manipulation is

relatively easy on account of the fact that one does not have to worry

about the bore of the tube. But the same general rule about not having

thick and thin spots in contact, and making all changes in diameter on a

taper if possible instead of abruptly, applies here. Thick pieces will

cool and contract at different rates from thin ones, and cracks are

likely to develop where they join. Work which has been formed with any

tool must always be heated to the softening point afterward before

allowing it to cool in order to remove the stresses caused by the

contact of the tool with the hot glass.

When it is necessary to join a piece of rod to the side of a piece of

tubing, the end of the rod is made very hot while the wall of the tube

at the spot desired is heated to just below the softening temperature.

The rod can then be pressed into firm union with the tube and drawn a

little to remove the excess of glass without deforming the tube.

MENDING STOPCOCKS

=Mending the Plug.=--The plug of the stopcock occasionally falls out and

is broken. If the break is in the main part of the plug, nothing can be

done except to search for a spare plug of suitable size and grind it to

fit, as described below. If only the little cross-piece at the end is

broken off, it can easily be replaced. In most ordinary stopcocks the

plug is solid, but the little handle is hollow. What has been said above

regarding care in heating and cooling glass rod applies with especial

force here. It is usually best to wind the whole of the plug with

several thicknesses of asbestos cord, leaving bare only the end where

the handle is to be joined. This diminishes the danger of cracking the

plug by too rapid heating, and also makes it more comfortable to hold. A

piece of rather thick-walled tubing of suitable diameter is chosen,

drawn out so as to have a suitable taper (taking care to heat enough of

the tube so that the capillary tail has good wall-thickness and

strength), and then a corresponding taper is drawn to form the other

side of the handle. The result is shown in Fig. 15, a. The capillary

tail is now heated and bent back to form a handle which will be in the

same straight line as the axis of the plug (b, Fig. 15) and the main

part of the tube drawn off at the dotted line, making a neat seal at

that point. The broken end of the plug is now slowly warmed in the smoky

flame, the heat gradually increased by a gentle stream of air from the

bellows, and the point at which this handle is to be attached finally

brought to the temperature at which the glass flows freely. In the mean

time, the little handle has been warmed almost to the softening point.

It is now quickly pushed into place (c, Fig. 15), taking care that its

axis is parallel to the hole in the plug, and then drawn away from the

plug just enough to make a graceful neck instead of the bulging one

indicated by the arrow in the figure. With a fine pointed flame the

little tail is now drawn off at the point indicated by the dotted line

(c, Fig. 15) and the whole carefully annealed. If necessary, the

handle can be blown a little before the tail is removed. Local heating

and blowing at the point where the handle joins the plug is often

necessary in order to make a smooth job.

=Regrinding.=--This is sometimes necessary to make stopcocks tight, when

the grinding has not been properly done in the factory. For this, a very

little fine flour of emery or carborundum is the best and quickest. If

this is not at hand, some clean sand may be ground in an agate mortar,

and if possible sieved. Only material which passes the 100-mesh sieve

should be used. It will be ground still finer in the process. For the

final polishing, a little infusorial earth or even kaolin will do.

The surface to be ground is moistened with water and dusted over with a

little of the abrasive. The plug is now inserted in the stopcock, and

turned with a gentle pressure. This turning should be in the same

direction for several revolutions, then in the opposite direction for

several more revolutions, etc. As the abrasive becomes finer during the

grinding, a little more may be added if necessary. In general, only a

little grinding will be required, and one small pinch of carborundum or

emery will be ample. The beginner usually grinds too much, and with too

coarse material. As the grinding surface becomes dry, water is added

drop by drop, and the grinding continued until the abrasive seems to be

reduced to an impalpable powder, most of which has been squeezed out of

the stopcock. The two surfaces in the stopcock are usually grinding upon

each other at this stage, and inspection will show whether the contact

between them is uniformly good. If not, the grinding must be continued

with a little fresh abrasive. If contact appears to be good, the

surfaces are ground together for a little with practically no abrasive,

so as to polish them, and the joint is then washed out and tested.

In grinding in a new plug to replace a broken one, the plug selected

should have practically the same taper as the seat into which it is to

be ground, and should be a very little too large. Care must be taken to

so distribute the abrasive material as to grind mostly on the places

where the plug fits tightly.

=Sealing on a New Tube.=--It frequently happens that one of the tubes of

the stopcock is broken off close to the cock itself, and a new one must

be joined to the stub of the old one. With care, this may often be

successfully done even where the break is within 1/4 inch of the

stopcock. The first step is to clean and dry the stopcock, remove the

plug, cork the open ends of the stopcock sleeve and the other tube, and

wind a couple of layers of asbestos cord carefully over the sleeve and

the most of the corks which close it. A suitable tube, having as near as

possible the same diameter and wall strength as the one broken off, is

selected and a piece the desired length cut off. The broken end of the

tube on the stopcock is now squared off as well as possible, by cutting

or by heating and drawing off the projections, and the new tube sealed

on, usually with the first method (Exercise No. 1). If the break is very

close to the stopcock, very little reheating and blowing can be done, on

account of the danger of getting the stopcock sleeve out of shape, and

the work must be heated very slowly to prevent cracking. The main

reliance is then placed on making a good joint when the tubes are

brought together, and then drawing out this joint a little, at once, to

get an even wall.