First Method--Making a Gas-washing Tube

First Method--Making a Gas-washing Tube

This first method can be used whenever one can work through an open end

opposite to the end of the tube where the joint is to be made. To

illustrate it, take a piece of rather thin-walled tubing, about 3/4 inch

in diameter, and some pieces of rather strong tubing a little less than

1/4 inch in diameter. Draw off the large tube in a short cone, then draw

off the tail as in the making of the bulb on the end of the tube, blow

out the little lump slightly, shrink the whole cone a little and blow

gently to form a rounded end like that on a test-tube, with walls about

the thickness of those of the rest of the tube. Cut this tube to a

suitable length, say about six inches, and provide two corks which will

fit the open end of it. Now cut a piece of the small tubing of the

proper length to form the piece which is to be inside the large tube.

For practice purposes, this piece should be about an inch shorter than

the large tube. Flange one end of this tube a little, and anneal the

flange well in the smoky flame. Bore one of the corks so that a piece of

the small tubing will fit it, and cut a couple of notches in the side of

this cork so that air can pass between it and the glass. Pass a short

piece of the small tubing through this cork, and attach the flanged

piece of small tube to this by means of a short piece of rubber tubing,

so that when the whole is inserted in the large tube it is arranged as

in a, Fig. 11. The piece of glass tubing projecting out through the

cork is now cut off so as to leave an end about 1/2 inch long when the

cork is firmly seated and the inner tube pushed into contact with the

center of the end of the large tube, as shown in the drawing. Care

should be taken that the little rubber tube which joins the two pieces

is arranged as in the figure; i.e., most of it on the piece of tubing

which passes through the cork, and very little on the other piece, so

that when the cork is removed after the small tube has been sealed

through the large one, the rubber tube may easily come with it. Select a

short piece of the small tubing of suitable length for the piece which

is to be on the outside of the large tube as a continuation of the

piece inside, and another piece for the delivery tube. A small bulb may

be blown in the latter at a point about 2-1/2 inches from the closed

end, and the open end cut off about 1-1/2 inches from the bulb. A cork

or cork-boring of suitable size to stopper the small tube is prepared,

and laid ready with the other (unbored) cork for the large tube.

When everything is in readiness, the rounded end of the large tube is

slowly heated until it softens and joins firmly to the small tube

inside. After it has shrunk down well, it is blown out to its original

size, placing the whole end of the large tube, cork and all, in the

mouth. Now with a fine-pointed flame the glass covering the end of the

small tube is heated to the softening temperature, and then is blown out

to an excrescence by blowing on the end of the small tube which passes

through the cork. The end of this excrescence is heated and blown off in

the usual way, so as to leave the small tube sealed on the inside of the

large one and opening through it into this short tube which has been

blown out. The end of the small tube which passes through the cork is

now closed with the cork prepared for it, and the short outer tube is

joined to the tube that has just been blown out, so that the joint

appears like b, Fig. 11. Use the first method (Exercise No. 1) for

this joint. Reheat the whole of the end of the tube nearly to the

softening temperature, anneal it a little, and allow to cool a few

seconds until well set. Now remove the cork, short glass tube and rubber

tube from the open end of the large tube and insert the solid cork in

their place. Warm the joint and the whole of that end of the tube again

carefully up to about the softening point, then seal on the side tube

for the delivery of the gas in the usual way, taking care that the whole

of the end and the joint are kept warm meanwhile. When thoroughly

sealed, the delivery tube is bent up parallel to the tube through which

the gas enters, and then out at right angles to it, as shown in c. The

whole of the end of the tube is now cautiously reheated and then cooled

slowly to anneal it.

The cork may now be removed from the open end of the large tube, this

end heated in a large flame, caught together with a scrap of glass

tubing and drawn off into a cone so that the base of the cone is about

opposite the end of the inner tube. The lump of glass is drawn off the

point of this cone and it is reblown to form a rounded end, as

previously described.

After this cools, the tube through which the gas enters may be heated at

the proper point and bent at right angles to form the finished apparatus

as shown in d. The ends of the small tube are cut off square and

fire-polished.

=Discussion.=--After the joint has once been made, great care must be

taken that it is kept hot during all the subsequent manipulations, and

if it becomes somewhat cool at any time it must be reheated very slowly.

It is obvious that the rate of heating and cooling of the inner tube

will be slower than that of the outer tube, and this will readily

produce stresses which tend to crack the tube at the joint. The amount

of heating and cooling which such a joint will stand depends upon its

form. The beginner should examine such a joint on regular factory-made

apparatus, and note the uniformity of wall-thickness and the "clean-cut"

appearance of the joint, as a model for his imitation. A ragged joint,

where the line of joining of the inner and outer tubes wavers instead of

going squarely around the tube, is almost sure to crack during the

cooling and heating unless extra precautions are taken with it. The

presence of a small lump of glass at any point on the joint affords an

excellent starting place for a crack, as do also the points on a ragged

joint where the inner tube comes farther down on the outer tube than at

other points.

In order to insure a joint which is square and not ragged, it is

essential that the angle between the inner and outer tubes at the joint

be very nearly a right angle. For this reason the two tubes should not

be of too near the same size, or if this cannot be avoided, a small bulb

should be blown on the end where the joint is to be made. If this bulb

be made with the same wall-thickness as the rest of the tube, and

somewhat pear-shaped, it may be drawn out to the same size as the rest

of the tube, if necessary, after the joint has been made.

This method is used wherever possible in preference to the second method

(Exercise No. 9), as it is easier to get a good joint with it. It may

also be used where it is desired to seal the tube through the side of a

tube, or for a tube sealed through the wall of a bulb, as in a Geissler

potash bulb or similar apparatus. Where there is not space to join the

inner tube to the blowing tube by a rubber tube, this joint may be made

with a small piece of gummed paper, which can readily be broken when

desired.