For this exercise tubing of 1/4 inch diameter and moderately strong
walls is selected. A tail is drawn out on one end of the tube, and a
piece of tubing about nine or ten inches long is cut off. The tail
should be carefully drawn in the axis of the tube, and in the same
straight line with it, as it is to be used as a handle in assembling the
glass for the bulb. This tail must be long enough so that it can be
conveniently held in the left hand, as described on page 13, and rotated
about the same axis as the main tube. Holding the main tube in the right
hand and the tail in the left, the tube is rotated in a large flame so
that a piece of it, beginning where the tail stops and extending about
an inch to the right, may be uniformly heated to the highest temperature
at which it can be kept in shape. As soon as this temperature is
reached, the tube is removed from the flame, continuing the rotation and
taking care not to draw out the heated part, and gently blown. The
rotation is carefully continued during the blowing, holding the tube in
approximately a horizontal position. As soon as the tube has expanded a
little the tail is pushed gently toward the main tube, continuing the
gentle blowing. If this is properly done, the heated piece of tube will
become a short bulb of about double its original diameter, and about the
same wall thickness as the original tube. It will have somewhat the
appearance of a, Fig. 10, when properly manipulated.
The tube is now reheated as before, taking care this time that the
heating extends over all that part of the bulb to the right of the
dotted line in the figure, as well as part of the main tube adjoining.
If this heating has been properly placed, when the operation of blowing
and pushing together is repeated the result will be to lengthen the bulb
into a uniform cylinder, as shown in b, Fig. 10. Otherwise the result
will be a series of bulbs, as in c, Fig. 10, separated by thickened
ridges which will be almost impossible of removal later and will
disfigure the final bulb. This operation of heating, blowing and pushing
together is repeated several times, until the cylinder becomes as long
as can be conveniently handled (about 1-1/4 inches to 1-1/2 inches). If
more glass is needed than is then contained in the cylinder, the latter
may now be heated as a whole, and blown and pushed gently into a shorter
cylinder of a slightly greater diameter, and more glass then added as
before.
When enough glass has been collected for the bulb, it is all well heated
and blown gently a couple of times, pushing the mass together as
required, until a thick bulb like d, Fig. 10, is obtained. The tail
must now be removed at the point indicated by the dotted line. To do
this, a very fine flame is directed on the point where the tail joins
the bulb, and the tube well rotated as the glass softens at that point.
When sufficiently soft, the work is raised a little, so that the flame
instead of striking the glass squarely at the point indicated passes
below and tangential to it. The tail is now drawn off slowly, continuing
the rotation, raising the work just out of the flame whenever the thread
of glass drawn off becomes too thin, and lowering it again to the point
where the flame just touches it when the glass stiffens a little. By
this means the tail may be drawn off without leaving an appreciable lump
behind, as indicated in e and f, Fig. 10. When as much of the extra
glass has been removed as is practicable, the flame is brought to play
squarely upon the little lump left, the last of the tail removed, and
the lump heated and gently blown to a small excrescence on the main
bulb. The whole end of the latter is now heated until it begins to
shrink a little, and gently blown to make it uniform in thickness. The
whole bulb is then heated in a flame of the proper size, so that it all
may shrink to about two-thirds of its diameter. The flame must be very
carefully chosen and directed, so as to shrink all the bulb, right up to
the main tube, but not soften the latter. As soon as this stage is
reached, the bulb is removed from the flame, continuing the even
rotation, and blown to the desired size, preferably by a series of
gentle puffs following one another at very short intervals. During the
blowing, the main tube is held in a horizontal position, and any
tendency of the bulb to fall out of line is corrected by the rotation.
If the shape of the bulb or its size are not satisfactory, it may be
shrunk again and reblown. Such shrinking should begin in a large yellow
flame, with just enough air to give it direction. The amount of air may
be gradually increased as the bulb shrinks and the walls become thick
enough to bear it without collapsing. If the bulb starts to collapse at
any time, it must be immediately blown enough to regain its convex
surface, before the shrinking proceeds further.
=Discussion.=--In collecting the glass for the bulb, enough must be
gathered to give the walls the desired strength. Since the area of a
sphere is proportional to the cube of its diameter, it is evident that
doubling the size of a bulb diminishes the thickness of its walls to a
very large extent. The limit of diameter for a strong bulb on ordinary
1/4-inch tubing, collecting the glass as above, is about 1-1/2 inches,
and the beginner will do well not to blow his bulbs more than an inch in
diameter.
The collection of the glass is one of the most important parts of the
process. If the mass of glass be twisted, furrowed or ridged, or
lop-sided, it is very difficult to get a good, even, spherical bulb, no
matter how many times it is shrunk and blown. The greatest care should
therefore be taken to get a uniform cylinder, on the same axis as the
main tube; and to this end the rotation of the tube must be carried on
very evenly. For method of holding the tube, see page 14.
If a very large bulb is required, it will often be economical to seal on
the end of the tube a short piece of a large tube, provided with the
proper tail, and use the glass in the large tube for the bulb instead of
attempting to collect it from the small tube. In this case part of the
small tube will usually be included in the bulb, so that the joint comes
in the latter, and not where it joins the tube. As the amount of glass
carried on the end of the tube increases in weight and size the
difficulties of heating it uniformly, keeping it in the proper position
and handling it increase rapidly.
In collecting glass, it is usually best not to leave the part of the
cylinder next the tube with too thick walls. This is always the coolest
part during the preparation for blowing the bulb, consequently it does
not get blown out, and causes an ugly thickened appearance on that end
of the bulb.
If the bulb grows too long or pear-shaped, it may be easily shortened by
heating to the blowing temperature, and then blowing gently with the
main tube in a vertical position, and the bulb at the top of it. Gravity
will then shorten the bulb nicely.
The finished bulb should be a nearly perfect sphere, with the axis of
the tube passing through its center, and the portion of the tube
adjoining the bulb must not be distorted, twisted, or blown out. In
order to prevent the distortion of the tube, care must be taken that it
is never heated quite to its softening point during the process.