Alum. Alum (1/4 weight of cotton) is dissolved in hot water with

Alum. Alum (1/4 weight of cotton) is dissolved in hot water with

carbonate of soda crystals, or other alkali (1/4 weight of alum); work

cotton in the solution, steep for several hours or overnight. Then

well wash. Aluminium acetate solution as for silk (page 56) may be

used. After drying, the cotton may be passed through a fixing solution

of some alkali, for examples see page 50. Before mordanting with

alum, the cotton is often prepared with tannic acid.

Iron. Iron is usually employed as a "saddening" agent, i.e. the

cotton after dyeing is steeped in a cold solution of the mordant. A

further use is in dyeing black, when the cotton, after being prepared

with tannin, is steeped in a cold solution of Iron. This process by

itself gives a dark colour before any dye is used.

Tin. Tin is rarely used alone as a mordant for cotton but brightens

the colour in combination with other mordants.

Chrome. Chrome is used for browns and other colours with Catechu.

After boiling in a solution of the dye stuff, boil a short time in

chrome solution, this oxidizes the colouring matter of the Catechu.

Copper. Copper is sometimes added in small quantities to the dye

bath for brown or yellow to vary the shade.

Tannin (Tannic acid). Cotton and linen strongly attract tannin and

when prepared with it they are able to retain dyes permanently. Cotton

saturated with tannin attracts the dye stuff more rapidly, and holds

it. Tannic acid is the best tannin for mordanting as it is the purest

and is free from any other colouring matter; it is, therefore, used

for pale and bright shades. But for dark shades, substances containing

tannic acid are used, such as sumach, myrobalans, valonia,

divi-divi, oak galls, chestnut (8 to 10 per cent tannin),

catechu.

Cotton and linen are prepared with tannin after they have been through

the required cleansing, and, if necessary, bleaching operations. A

bath is prepared with 2 to 5 per cent of tannic acid of the weight of

the cotton, and a sufficient quantity of water. For dark shades, 5 to

10 per cent should be used. The bath is used either hot or cold. It

should not be above 60 deg.C. The cotton is worked in this for some

time, and then left to soak for 3 to 12 hours, while the bath cools.

It is then wrung out and slightly washed.

The following gives the relative proportions of the various substances

containing tannin:--1 lb. tannic acid equals 4 lbs. sumach, 18 lbs.

myrobalans, 14 lbs. divi-divi, 11 lbs. oak galls.

Examples from various recipes:

For 10 lbs. cotton use 12 ozs. tannic acid.

" 50 " " " 10 lbs. sumach.

" 40 " " " 10 lbs. "

" 20 " " " 2 lbs. yellow (or black) catechu.

" 20 " " " 3 lbs. catechu with 3 ozs. blue vitriol.

Some recipes soak the cotton 24 hours, others 48.